Navigation Menu 

|
Semiconductor Constants
This section includes information on properities of silicon, germanium, gallium arsenide, and other semiconductors.
- Properties of Si
|
Crystal Properties
|
|
|
Atoms/cm3
|
5.0e22
|
|
Atomic weight
|
28.086
|
|
Crystal
structure
|
Diamond
|
|
Density
|
~3e5
|
|
Lattice Constant
|
5.4310 A
|
|
Band structure Properties
|
|
|
Dielectric constant
|
11.9
|
|
Eff. Density of states (conduction, Nc)
|
2.8e19 cm-3
|
|
Eff. Density of states (valence, Nv
|
1.04e19 cm-3
|
|
Electron affinity
|
4.05
|
|
Minimum Indirect Energy Gap (300K)
|
1.12 eV
|
|
Minimum Direct Energy Gap
|
3.4 eV
|
|
Intrinsic Carrier concentration
|
1.45e10 cm-3
|
|
Intrinsic Debye length
|
24 um
|
|
Intrinsic resistivity
|
2.3e5 ohm-cm
|
|
Minority carrier lifetime
|
2.5e-3 s
|
|
Mobility (drift) (cm2/V-s)
|
1500(electron);450(hole)
|
|
Thermal Properties
|
|
|
Linear coefficient of thermal expansion
|
2.6e-6 (degC-1)
|
|
Melting point
|
1414 degC (estimated)
|
|
Boiling Point
|
2878degC
|
|
Specific heat
|
0.7 J/g-degC
|
|
Thermal conductivity @ 300K
|
1.5 W/cm-degC
|
|
Thermal diffusivity
|
0.99 cm2/s
|
|
Vapor Pressure (Pa)
|
1@1650degC; 1e-6@900degC
|
|
Other Properties
|
|
|
Hardness
|
1150 kg/mm2
|
|
Compressibility coefficient
|
1.0 cm2/dyne
|
|
Bulk modulus
|
9.8 dyne/cm2
|
|
Young’s modulus
|
1.3 dyne/cm2
|
|
Coefficient of thermal expansion
|
2.33 /degC
|
|
dn/dT
|
1.2 degC
|
|
Elastic constant, C11
|
1.656 dyne/cm2
|
|
Elastic constant, C12
|
0.639 dyne/cm2
|
|
Elastic constant, C44
|
0.795 dyne/cm2
|
|
Breaking strength, compression
|
4900-5600 Kg/cm2
|
|
Rupture modulus, bending
|
700-3500 Kg/cm2
|
- Properties of Ge
| Crystal structure |
Diamond |
| Auger recombination coefficient |
10-30 cm6/s |
| Debye temperature |
374 K |
| Density |
5.3234 g/cm3 |
| Dielectric constant |
16.2 |
| Effective electron masses ml |
1.6mo |
| Effective electron masses mt |
0.08mo |
| Effective hole masses mh |
0.33mo |
| Effective hole masses mlp |
0.043mo |
| Electron affinity |
4.0 eV |
| Lattice constant |
5.658 A |
| Optical phonon energy |
0.037 eV |
| Breakdown field |
˜105V cm-1 |
| Mobility electrons |
=3900 cm2 V-1s-1 |
| Mobility holes |
=1900 cm2 V-1s-1 |
| Diffusion coefficient electrons |
=100 cm2 s-1 |
| Diffusion coefficient holes |
=50 cm2 s-1 |
| Electron thermal velocity |
3.1·105m s-1 |
| Hole thermal velocity |
1.9·105m s-1 |
| Infrared refractive index n |
4.00 |
| Radiative recombination coefficient |
6.4·10-14 cm3/s |
| Bulk modulus |
7.5·1011 dyn cm-2 |
| Melting point |
937 °C |
| Specific heat |
0.31 J g-1 °C-1 |
| Thermal conductivity |
0.58 W cm-1 °C-1 |
| Thermal diffusivity |
0.36 cm2s-1 |
| Thermal expansion, linear |
5.9·10-6 °C -1 |
| Bulk modulus |
7.5·1011 dyn cm-2 |
| Melting point |
937 °C |
| Specific heat |
0.31 J g-1 °C-1 |
| Thermal conductivity |
0.58 W cm-1 °C-1 |
| Thermal diffusivity |
0.36 cm2s-1 |
| Thermal expansion, linear |
5.9·10-6 °C -1 |
| Bulk modulus |
7.5·1011dyn cm-2 |
| Density |
5.323 g cm-3 |
| Cleavage plane |
{ 001 } |
| Elastic Modulus C11 |
12.60·1011 dyn cm-2 |
| C12 |
4.40·1011 dyn cm-2 |
| C44 |
6.77·1011 dyn cm-2 |
|
- Properties of GaAs
| Crystal structure |
Zinc Blende |
| de Broglie electron wavelength |
240 A |
| Debye temperature |
360 K |
| Density |
5.32 g cm-3 |
| Dielectric constant (static ) |
12.9 |
| Dielectric constant (high frequency) |
10.89 |
| Effective electron mass me |
0.063mo |
| Effective hole masses mh |
0.51mo |
| Effective hole masses mlp |
0.082mo |
| Electron affinity |
4.07 eV |
| Lattice constant |
5.65325 A |
| Optical phonon energy |
0.035 eV |
| Energy gap |
1.424 eV |
| Energy separation (EΓL) between Γ and L valleys |
0.29 eV |
| Energy separation (EΓX) between Γ and X valleys |
0.48 eV |
| Energy spin-orbital splitting |
0.34 eV |
| Intrinsic carrier concentration |
2.1·106 cm-3 |
| Intrinsic resistivity |
3.3·108 Ω·cm |
| Effective conduction band density of states |
4.7·1017 cm-3 |
| Effective valence band density of states |
9.0·10-18 cm-3 |
| Breakdown field |
≈4·105 V/cm |
| Mobility electrons |
≤8500 cm2 V-1s-1 |
| Mobility holes |
≤400 cm2 V-1s-1 |
| Diffusion coefficient electrons |
≤200 cm2/s |
| Diffusion coefficient holes |
≤10 cm2/s |
| Electron thermal velocity |
4.4·105 m/s |
| Hole thermal velocity |
1.8·105m/s |
| Infrared refractive index |
3.3 |
| Radiative recombination coefficient |
7·10-10 cm3/s |
| Bulk modulus |
7.53·1011 dyn cm-2 |
| Melting point |
1240 °C |
| Specific heat |
0.33 J g-1°C -1 |
| Thermal conductivity |
0.55 W cm-1 °C -1 |
| Thermal diffusivity |
0.31cm2s-1 |
| Thermal expansion, linear |
5.73·10-6 °C -1 |
| Bulk modulus | 7.53·1011
dyn cm-2 | | Density | 5.317 g cm-3 |
| Cleavage plane | {110} | | Piezoelectric constant | e14=-0.16
C m-2 |
| C11 | 11.90·1011 dyn/cm2 |
| C12 | 5.34·1011 dyn/cm2 |
| C44 | 5.96·1011 dyn/cm2 |
- Properties of Select Binary Semiconductors
|
Parameter
|
AlP
|
AlAs
|
AsSb
|
GaP
|
GaAs
|
GaSb
|
InP
|
InAs
|
InSb
|
|
Direct
Energy Gap
(eV@300K)
|
Γ15- Γ1
|
3.62
(77K)
|
3.14
|
2.22
|
2.78
|
1.424
|
0.70
|
1.34
|
0.356
|
0.180
|
|
Direct Energy Gap
(eV @0K)
|
Eg = Ego - αT2/(T+β)
|
Eg
|
2.52
|
2.239
|
1.687
|
2.338
|
1.519
|
0.810
|
1.421
|
0.420
|
0.236
|
|
α (10-4eV/K)
|
3.18
|
6.0
|
4.97
|
5.771
|
5.405
|
3.78
|
3.63
|
2.50
|
2.99
|
|
β
|
588
|
408
|
213
|
372
|
204
|
94
|
162
|
75
|
140
|
|
Indirect Energy Gap
|
Γ15- X1
|
2.45
|
2.14
|
1.63
|
2.268
|
1.804
|
1.25
(10K)
|
2.74
|
--
|
--
|
|
Temperature
dependence or direct and indirect energy gap
|
dEd/dT
dEind/dT
|
-3.6
|
-5.2
-4.0
|
-3.5
|
-4.5
-5.2
|
-3.9
-2.4
|
-3.7
|
-2.9
-3.7
|
-3.5
|
-2.8
|
|
Indirect Energy Gap
|
Γ15- L1
|
--
|
--
|
--
|
--
|
1.81
(110K)
|
0.81
|
1.74
|
--
|
--
|
|
Lattice Constant
(Å)
|
5.467
|
5.660
|
6.136
|
5.4512
|
5.6532
|
6.0959
|
5.8687
|
6.0583
|
6.4794
|
|
Density (gm cm-3)
|
2.40
|
3.70
|
4.26
|
4.138
|
5.3161
|
5.6137
|
4.81
|
5.667
|
5.7747
|
|
Melting Point (K)
|
2823
|
2013
|
1338
|
1740
|
1513
|
985
|
1335
|
1215
|
800
|
|
Coefficient of
Thermal Expansion 10-6/°C (@300K)
|
4.5
|
4.9
|
4.0
|
4.5
|
6.86
|
7.75
|
4.75
|
4.52
|
5.37
|
|
Thermal
Conductivity
(W cm-1 K-1)
|
0.9
|
0.8
|
0.57
|
0.77
|
0.46
|
0.39
|
0.68
|
0.273
|
0.166
|
|
Refractive index n
(near Eg)
|
3.03
|
3.18
|
3.4
|
3.45
|
3.65
|
3.82
|
3.41
|
3.52
|
4.00
|
|
Dielectric constant
|
static ε(0)
|
9.8
|
10.06
|
12.04
|
11.1
|
12.91
|
15.69
|
12.61
|
15.15
|
17.7
|
|
high f ε(∞)
|
7.54
|
8.16
|
10.24
|
9.08
|
10.9
|
14.44
|
9.61
|
12.25
|
15.68
|
|
(1/n)*(dn/dT)*(K-1) x10-5
|
3.5
|
4.6
|
3.5
|
2.5
|
4.5
|
8.2
|
2.7
|
6.5
|
0.12
|
|
Elastic Compliances
(10-12 cm2 dyne-1)
|
S11
|
1.090
|
1.070
|
1.696
|
0.973
|
1.176
|
1.582
|
1.650
|
1.945
|
2.443
|
|
S12
|
-0.350
|
-0.320
|
-0.562
|
-0.298
|
-0.365
|
-0.495
|
-0.594
|
-0.685
|
-0.863
|
|
S44
|
1.630
|
1.840
|
2.453
|
1.419
|
1.684
|
2.314
|
2.170
|
2.525
|
3.311
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
Properties of Ternary Semiconductors
|